Engineer_Drew
I am working on a hss frame. The position the part arrives in I have some 3F welds and 1G (flare bevels) to complete. Currently I am doing it in separate moves but have been trying to get a compound weld to accomplish it for me. Given the change in torch angle that happens when making the turn I regularly get an joint speed error. It is possibly that I was making my points too close to each other and not programming the corner correctly.
In general is this a successful tactic or am I better off just keeping them as separate paths?
Reply 0 0
Marcus Yakawich Marcus Yakawich
Hi Drew,
For a weld transition, I see two approaches.
 
Option 1: Break the transition into two separate welds. This is the quickest route, but will require an extra start/stop which may be undesirable.
 
Option 2: Transition the weld using WeldThruL's (QTY 3). As you've already noticed, this option will likely take more time to tweak to avoid too much reorienting in the transition. I'd recommend one of the waypoints (1) prior to the transition, one waypoint (2) at the transition point, and the last (3) after the transition. I'd recommend spacing the WeldThruL's somewhere between 1/2"-1" apart (the more spacing, the better). I'd also play with the tool spin to minimize the amount of reorienting between these three waypoints which will assist in avoiding speed errors. You can update the weld process at the center/transition point (2) for transitioning between the weld positions.
 
2026-01-13_10-17-44.jpg
 
An example of this type of programming can be seen here (academy link). I hope this helps. As always, we can chat through your specific application details further if needed on a phone call. I can connect you with Christian Atkins, whom covers your area.

Marcus Yakawich, CRAW-T, CWI
Vectis Automation - Product Manager
Reply 0 0
Engineer_Drew
Thanks Marcus. That is helpful and we are going with option 1 for now. We plan to re orient the parts in the next few weeks and that should help us weld the corners better.